order Inquiries

ULTRA SUPER PUNCHINGTM TENSILE TEST

1.Purpose Tensile strength test for perforated metal.
2.Samples to be tested ①SUS304 and ②&③SUS316L.
3.Test Method
Photo of test condition in shown in Picture1.

◎Tensile Test
Testing equipment : Shimazu Universal Tester type : AG-X300kN(E2-020)
Test Conditions

  1. Number of test pieces : 6 pieces
  2. Environmental temperature : Room temperature 23℃±5℃)
  3. Testing speed : 30% of width (mm)/min
  4. Dimensions of test piece
    1. 25mm width x 280mm length
    2. Thickness ①3t(SUS304)②3t(SUS316L)③6t(SUS316L)

Two patterns, which are Staggered and Reverse Staggered, were tested

4.Result The test results are summarized in the following pictures and table.
Picture1. Test condition.
Picture2. Test piece after the test.
Chart3. Stress-Strain Curve.
Table1. Result of tensile test.
 

Result of tensile test.

Table 1

Chart   Material Thickness Number of
test piece
Dimensions of test piece Environmental
temperature
Ultimate Strength
(N)
Width Thickness
(mm) (mm)
SUS304 3 Staggered
Ⓐ-①
24.98 2.92 RT
(23℃)
24525
SUS316L 3 Staggered
Ⓐ-②
24.95 2.84 21320
SUS316L 6 Staggered
Ⓐ-③
24.92 5.79 46874
SUS304 3 Reverse Staggered
Ⓑ-①
24.94 2.92 22914
SUS316L 3 Reverse Staggered
Ⓑ-②
24.94 2.85 19055
SUS316L 6 Reverse Staggered
Ⓑ-③
24.94 5.84 54314
  Applicable Test Standard : JIS Z224(11)   # of the test equipment : E2-020
Remarks Testing speed : 30%/min   Room temperature : 23℃± 5℃

 

 
Ⓐ Stress-Strain Curve (Staggered)
Ⓑ Stress-Strain Curve (Reverse Staggered)

Click HERE to download PDF English catalog.
mm notation